Volume discount: 5 pcs 2% · 10 pcs 3% · 25 pcs 5%The scratch is visible to the eye but not in the report: how to measure directly on the microscope imageWhy a two-point measurement of a bore often shows the wrong diameter, and how a three-point micrometer solves itThree seconds instead of half a minute: how core temperature checks become a routine that actually gets doneA Hundred Bearing Seats per Shift: Read the Deviation Directly Instead of Calculating the DiameterThe hole measures correctly at the mouth but is tapered further in: how to find the fault without cutting up the partOne Second Is Enough to Tell Whether the Core Temperature PassesThree contact points give a bore measurement that doesn’t depend on who is holding the instrumentWhen the measurement has to be taken from an image: how automatic magnification reading makes microscope measurement traceableThe vernier caliper that keeps reading correctly when the scale is covered in coolant and chipsThree measuring points give the right bore size when the operator’s hand would otherwise decide the resultVolume discount: 5 pcs 2% · 10 pcs 3% · 25 pcs 5%The scratch is visible to the eye but not in the report: how to measure directly on the microscope imageWhy a two-point measurement of a bore often shows the wrong diameter, and how a three-point micrometer solves itThree seconds instead of half a minute: how core temperature checks become a routine that actually gets doneA Hundred Bearing Seats per Shift: Read the Deviation Directly Instead of Calculating the DiameterThe hole measures correctly at the mouth but is tapered further in: how to find the fault without cutting up the partOne Second Is Enough to Tell Whether the Core Temperature PassesThree contact points give a bore measurement that doesn’t depend on who is holding the instrumentWhen the measurement has to be taken from an image: how automatic magnification reading makes microscope measurement traceableThe vernier caliper that keeps reading correctly when the scale is covered in coolant and chipsThree measuring points give the right bore size when the operator’s hand would otherwise decide the result

The instrument measures HL, everything else on the display is converted

Published 25 August 2026 at 19:42

The display can show hardness in six different scales: HL, HB, HRC, HV, HRB and HS. It looks like six measurements. It isn’t — it’s one measurement and five conversions, and the difference is worth understanding before a value gets written into a protocol.

Digital hardness tester with impact device D and conversion to HB, HRC, HV, HRB and HS

What it is

A portable digital hardness tester with an external impact device.

  • Measuring ranges: HL 174-900, HB 20-655, HRC 19.6-68, HV 80-940, HRB 13.5-101.7, HS 32.5-99.5
  • Accuracy ±0.5% at HL 800
  • Minimum spherical surface radius 30 mm, carbide tip
  • Complies with DIN 50156 and ISO 16859
  • Memory for 10,000 measured values, USB data output
  • 133 x 75 x 29 mm, 260 grams, external impact device D
  • Supplied with a factory measurement certificate

Why HL is the value the instrument actually knows

The method is based on rebound. An impact body with a carbide tip is shot against the surface with a defined energy, and the instrument measures the ratio between the velocity before and after impact. That ratio is expressed as an HL value. Harder materials absorb less energy and produce a faster rebound.

The other scales are tables. HRC, HB, HV and the others are defined through entirely different tests — an indentation that is made and measured, not a rebound. Going from HL to HRC therefore means looking up what an HL value usually corresponds to, and that relationship has been derived empirically for common steels.

Which is why the conversion is material-dependent. The rebound is affected not only by hardness but also by the material’s elasticity. Two materials that produce the same HL value may well give different HRC values on a bench tester, because they spring back differently. The conversion works well within the material group it was developed for — and less well outside it.

The practical conclusion is simple: measure in HL and stick to the same scale internally, and every comparison stays valid. If a value needs to be reported in HRC because that’s how the specification is written, note that it is a converted value. In a dispute, the matter is settled on a bench tester — but by then you already know what to look at.

Two limitations that are easy to run into

Minimum spherical surface radius 30 mm. On a strongly curved surface, the impact body doesn’t seat properly, so the rebound isn’t representative. That applies to small shafts, round bars and radii — exactly the kind of detail you’d want to check. Support rings for curved surfaces can shift that limit, but it doesn’t work straight off.

The part must sit firmly and have mass. The rebound method assumes the workpiece absorbs the impact without moving itself. A light or loosely resting part springs away, absorbs energy and gives a reading that’s too low — consistently, and without anything looking obviously wrong.

Three typical use cases

  • Incoming inspection: verifying that delivered material and heat-treated parts are within spec.
  • Large and assembled parts: where a bench tester is out of the question and the test has to come to the workpiece.
  • Follow-up: series of measurements in memory and via USB, where the trend over time is what matters.

Why it pays off

Incorrect hardness is almost always discovered too late, and the cost lands in the machining and assembly already carried out. A test that takes seconds and can be done anywhere moves that check to a point where a mixed-up batch still only costs the material.

The fact that the instrument also stores ten thousand values and outputs them via USB makes the difference between a spot check and documentation. And for anyone who understands that HL is the measurement and the rest is conversion, the figures also become comparable — which is the whole point of saving them.